华南理工大学学报(自然科学版) ›› 2011, Vol. 39 ›› Issue (3): 1-7.doi: 10.3969/j.issn.1000-565X.2011.03.001

• 化学化工 •    下一篇

蔗渣浆纤维模塑装饰建筑材料的制备与性能

韩文佳1 陈克复1 杨仁党1,2 杨飞1 黄良辉1 高文花1   

  1. 1.华南理工大学 制浆造纸工程国家重点实验室∥广东省造纸技术与装备公共实验室,广东 广州 510640;2.华南理工大学 亚热带建筑科学国家重点实验室,广东 广州 510640
  • 收稿日期:2010-03-31 修回日期:2010-09-10 出版日期:2011-03-25 发布日期:2011-02-01
  • 通信作者: 韩文佳(1984-),男,博士生,主要从事植物纤维资源的资源化利用研究 E-mail:hwj200506@163.com
  • 作者简介:韩文佳(1984-),男,博士生,主要从事植物纤维资源的资源化利用研究
  • 基金资助:

    国家“十一五”科技支撑项目(2007BAF25B02—3);华南理工大学亚热带建筑科学国家重点实验室开放基金资助项目(2010KB21)

Preparation and Properties of Bagasse Fibre-Molding Decorative Building Material

Han Wen-jiaChen Ke-fu  Yang Ren-dang1,2   Yang Fei  Huang Liang-hui  Gao Wen-hua1   

  1. 1.State Key Laboratory of Pulp and Paper Engineering}f Guangdong Public Laboratory of Paper Technology and Equipment.South China University of Technology ,Guangzhou 5 10640,Gunangdong,China;2.State Key Laboratory ofSubtropical Building Science,South China University of Technology,Guangzhou 510640,Guangdong,China
  • Received:2010-03-31 Revised:2010-09-10 Online:2011-03-25 Published:2011-02-01
  • Contact: 韩文佳(1984-),男,博士生,主要从事植物纤维资源的资源化利用研究 E-mail:hwj200506@163.com
  • About author:韩文佳(1984-),男,博士生,主要从事植物纤维资源的资源化利用研究
  • Supported by:

    国家“十一五”科技支撑项目(2007BAF25B02—3);华南理工大学亚热带建筑科学国家重点实验室开放基金资助项目(2010KB21)

摘要: 以天然蔗渣浆纤维为原料,利用模塑热压工艺复合成形,得到物理性能优良的纤维模塑装饰建筑材料.借助拉伸性能测试、热重分析、FT-IR等研究了影响该材料力学性能的因素.研究表明:该材料的拉伸性能主要受增强剂和阻燃剂添加量,干燥温度、时间和压力的影响;随着阻燃剂添加量的增加,材料的拉伸性能明显降低;最佳干燥温度为160℃,干燥时间为4 min;在一定施压范围内,随着干燥压力的提高,材料拉伸性能提高,合适的干燥压力为30kN.热重分析和FT-IR分析表明,材料制备过程中蔗渣浆纤维未发生明显的热解反应,化学成分也未发生变化,因此材料的微观结构对其拉伸性能具有重要影响.最后利用SEM、AFM等对材料的表面微观结构进行了表征.

关键词: 蔗渣纤维, 模塑, 装饰建筑材料, 热解性能, 拉伸特性

Abstract:

 Molding decorative building material with excellent physical performances was prepared from natural bagasse fibers via the hot forming process of fiber molding.Then,based on the tensile test,TGA and FT-IR analysis,the factors affecting the mechanical properties of the material were investigated.The results indicate that the tensile performance of the material is mainly affected by the dosages of flame retardant and reinforcing agent,the drying temperature,the drying time and the pressure,that,with the increase of flame retardant dosage,the tensile perfor-mance greatly degrades,that the optimal drying temperature and time are respectively determined as 160℃ and 4min,and that,in a certain pressure range,the tensile performance improves with the drying pressure at an optimal value of 30kN.Moreover,it is found from TGA and FT-IR analysis that,as there is no obvious thermal decomposition and chemical structure change of bagasse fibers during the preparation,the microstructure of the prepared material plays an important role in the tensile performance.In addition,the surface microstructure of the material was analyzed by means of SEM and AFM.

Key words: bagasse fiber, molding, decorative building material, pyrolysis performance, tensile characteristics